Ash glazes are the oldest glazes in the world and the only ones where the main flux is something you can collect from your own fireplace. The catch is variability: wood ash is mostly calcium oxide, but the exact proportion depends on the tree species, the soil, the part of the tree that burned and how completely it burned. This recipe gives a working range and the procedure for dialling in a new batch.
H 15 · Ø14 / Ø16 / Ø7 cm
Base
A triaxial ash glaze for cone 10 reduction, using washed wood ash from a hardwood fire as the main flux. Ash is a variable material: every batch of ash is a slightly different flux, which is why the recipe is written as a range and the first firing of each new ash batch is a test.
| Material | Parts | Share |
|---|---|---|
| Washed Hardwood Ash | 40 | 39.2% |
| Custer Feldspar | 30 | 29.4% |
| EPK Kaolin | 15 | 14.7% |
| Silica (SiO₂) | 10 | 9.8% |
| Whiting (CaCO₃) | 5 | 4.9% |
| Red Iron Oxide (Fe₂O₃) | 2 | 2.0% |
| Total charge | 102 |
Fired surface
A glossy, slightly milky green-brown with tiny ash specks and a texture that runs from smooth where the glaze is thick to dry and orange-peeled where it is thin. Where it pools it is a deep green; where it breaks on a rim it is a warm cream.
Collecting and washing the ash
Hardwood ash is better than softwood ash: it is higher in calcium and contains fewer of the soluble potassium salts that make a glaze foam and craze. Collect from a fire of oak, maple, ash or fruitwood. Do not use ash from a fire that burned painted wood, plywood, charcoal briquettes or treated timber — those bring in lead, zinc and heavy metals.
Wash the ash in a bucket: cover with three times its volume of water, stir, let it settle for two hours, and pour off the water. Repeat three times. The washing removes the soluble alkalis, which are what make unwashed ash glazes foam and pinhol, and it drops the flux strength by about 15 percent. Dry the washed ash on a tray before weighing it.
Adjusting the recipe to a new batch
Start with 40 parts ash and fire a test tile on the first firing of every new batch. If the glaze is a dry, unmelted matte, increase the ash to 45 and reduce the feldspar to 25. If it is over-fluxed and has run off the tile, reduce the ash to 35 and increase the kaolin to 18. Work in 5-part steps and record the result each time.
The ash also carries iron and trace manganese, which is why the recipe's own iron addition is only 2 percent. A dark-coloured ash will give a browner glaze at the same addition; a very pale ash will give something closer to a celadon. Keep a photograph of each batch of fired tests on the bucket.
Sieving and the speckle decision
Ash glazes can be sieved to 40 mesh for a heavy speckle, 80 mesh for a light speckle, or 100 mesh for a nearly smooth surface. The specks are unburnt carbon and insoluble mineral particles and they are the signature of an ash glaze, but too much speckle reads as a defect on a fine piece. Sieve to 80 for anything you intend to sell.
Crush the ash lightly with a rolling pin before sieving; ash from a cold fire is often in soft lumps that will not pass through the sieve at all and will fire as large pale blisters on the glaze.
Firing, and why ash likes a long firing
Ash glazes benefit from a slower firing than a standard recipe: they contain a lot of calcium and very little boron or alkali, so they need time at the top temperature to melt fully and heal the surface. Soak for 30 minutes at cone 10 rather than 15.
Fire in medium reduction. Ash glazes in oxidation are flat and often yellow-brown; reduction brings out the green-brown and the depth. The same slow cool that suits iron satin — four to six hours down to 900 degrees — also suits ash, and gives it the faint blue-green haze that appears in the pooled areas on a good firing.
Steps
- Collect hardwood ash only; no painted, treated or briquette ash.
- Wash the ash three times with three volumes of water each time, then dry it on a tray.
- Crush the dry ash lightly and sieve it to 80 mesh.
- Weigh the ash, feldspar, kaolin, silica, whiting and iron oxide and combine dry.
- Add water, mix for eight minutes and adjust to 1.44 specific gravity.
- Fire a test tile before committing a load, on the first firing of every new ash batch.
- Adjust ash in 5-part steps against the kaolin if the melt or the colour is off, and record each result.
- Apply to the main work at 1.0 mm and fire to cone 10 in medium reduction with a 30-minute soak.
- Cool over four to six hours to 900 degrees, then let the kiln fall naturally.
Where it goes wrong
- Using ash from a fire that burned painted or treated wood. It carries heavy metals into a food surface.
- Skipping the washing. Unwashed ash glazes foam, pinhole and craze badly.
- Not testing a new ash batch. Ash varies enough between batches to move the melt point by a cone.
- Sieving to 40 mesh on a fine piece. The speckle reads as a defect at that scale.
- Firing in oxidation. The colour goes flat and yellow-brown.
| Symptom | Cause |
|---|---|
| Glaze did not melt, dry and matte | the ash was under-fluxing for this batch; raise ash to 45 and lower feldspar to 25. |
| Glaze ran off the test tile | the ash was over-fluxing; lower ash to 35 and raise kaolin to 18. |
| Heavy foaming and pinholing | the ash was not washed, so soluble alkalis are still present. |
| Large pale blisters on the fired surface | ash lumps that never passed the sieve; crush and re-sieve the batch. |
| Colour is flat yellow-brown | fired in oxidation rather than medium reduction. |
Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.
Same cone — Cone 10
- Cooling in reduction: how 90 minutes of controlled cooling changes a glaze Stoneware
- Celadon at cone 10: colour from thickness, not from iron Porcelain
- Copper red: the reduction window is the whole recipe Porcelain
- Iron satin tenmoku: eight percent iron and a surface you can feel Stoneware
- Oil spot tenmoku: twelve percent iron and a long soak at the top Stoneware
- Shino: a glaze that is mostly feldspar and mostly technique Stoneware