Oil spots are formed when iron oxide in a fluid glaze comes to the surface during a long soak and crystallises as magnetite, then cools without re-dissolving. Everything in this recipe serves that one event: the 12 percent iron supplies the material, the 25 percent silica keeps the glaze fluid enough for the iron to move, and the bone ash steadies the melt so the soak can be long without the glaze running off the pot.
H 14 · Ø12.5 / Ø15 / Ø6.5 cm
Base
An oil spot tenmoku for cone 10 reduction: a high-iron base with enough silica to keep the surface fluid, fired so that iron crystals bloom out of the glaze as silver-brown spots. The spots are a firing event, not a recipe ingredient.
| Material | Parts | Share |
|---|---|---|
| Custer Feldspar | 35 | 35.0% |
| Silica (SiO₂) | 25 | 25.0% |
| EPK Kaolin | 14 | 14.0% |
| Red Iron Oxide (Fe₂O₃) | 12 | 12.0% |
| Whiting (CaCO₃) | 10 | 10.0% |
| Bone Ash (Ca₃(PO₄)₂) | 3 | 3.0% |
| Talc | 1 | 1.0% |
| Total charge | 100 |
Fired surface
A black-brown glaze covered with round, slightly raised spots that are silver-brown at the centre and darker at the edge. The spots are densest on the upper two thirds of a vertical pot and disappear near the foot where the glaze pools.
Why 12 percent iron does not make it metallic
Iron satin uses 8 percent iron and looks like a glaze; oil spot uses 12 percent and still looks like a glaze, because the extra silica and the bone ash keep the iron in solution rather than letting it go metallic. Remove the bone ash and the same recipe blisters and shows a metallic sheen. The bone ash is not decorative here, it is structural.
Above 14 percent iron the glaze stops being able to hold the iron at all and you get a crawling, blistering mess regardless of the soak. Twelve percent is close to the practical ceiling.
The soak is the whole technique
Fire to cone 10 and then hold for 45 to 60 minutes. The soak lets iron-rich material migrate to the surface and gather into droplets; on cooling, those droplets crystallise as magnetite spots. A 15-minute soak gives a plain dark tenmoku with no spots at all.
Soaking this long is a real strain on the kiln and on the glaze: the glaze must be fluid enough to move iron but viscous enough not to run off the pot. This is the reason for the 25 percent silica and the 3 percent bone ash. Do not soak past 75 minutes or the spots start to coalesce and the surface goes smooth and black.
Cooling and re-solution
Cooling too slowly lets the spots re-dissolve back into the glaze, which is the most common reason a well-soaked oil spot comes out plain. Cool from cone 10 to 1000 degrees in about 90 minutes to two hours — fast enough to freeze the crystals, slow enough not to crack the ware.
This is the opposite of what a copper red or a celadon wants in the same kiln, which is a practical scheduling problem: you cannot put an oil spot, a copper red and a celadon in the same load and have all three come out right. Oil spot wants a fast cool, copper red and celadon want a slow one.
Placement in the kiln
Spots form best on vertical surfaces in the upper part of the kiln, where the glaze is slightly hotter and the atmosphere is most active. Put tall forms on the top shelf and plates low, and expect plates to come out with far fewer spots because the glaze on a flat surface pools rather than flowing.
The glaze is unstable at cone 10 on a thin foot ring and will run. Leave a 5 mm unglazed foot and use a washed shelf with a thin coat of alumina wax. Pieces placed within 1 cm of each other can weld together at this iron level.
Steps
- Weigh the seven materials and combine dry, sieving the iron oxide to break up lumps.
- Add water and mix for eight minutes, then adjust to 1.46 specific gravity.
- Sieve through 80 mesh and let the bucket stand for one hour to fully wet out.
- Dip for two seconds to build 0.9 mm, or pour the interior and dip the exterior.
- Wipe a 5 mm foot ring clean and set the piece on a washed shelf with alumina wax.
- Load tall pieces on the top shelf and leave at least 1 cm between all pieces.
- Fire to cone 10 with medium reduction and soak for 45 to 60 minutes.
- Cool from cone 10 to 1000 degrees in 90 minutes to two hours; do not damper down further.
- Examine the spots cold; a warm oil spot still looks plain.
Where it goes wrong
- Soaking only 15 minutes. You get a plain dark tenmoku with no spots.
- Soaking past 75 minutes. The spots coalesce into a smooth black surface.
- Cooling slowly. The magnetite spots re-dissolve into the glaze.
- Firing oil spot, copper red and celadon in one load. They want opposite cooling rates.
- Loading pieces within 1 cm. At 12 percent iron the glaze will weld them together.
| Symptom | Cause |
|---|---|
| No spots at all on a correctly mixed glaze | the soak was too short, under 30 minutes at cone 10. |
| Spots formed but disappeared before opening | the cooling was too slow and the magnetite re-dissolved. |
| Surface is blistered with a metallic sheen | bone ash was left out or reduced below 2 percent. |
| Spots merged into a smooth black area | the soak was longer than 75 minutes. |
| Glaze ran onto the shelf and welded pieces together | applied too thick, or less than 1 cm clearance between pieces. |
Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.
Same cone — Cone 10
- Cooling in reduction: how 90 minutes of controlled cooling changes a glaze Stoneware
- Celadon at cone 10: colour from thickness, not from iron Porcelain
- Copper red: the reduction window is the whole recipe Porcelain
- Iron satin tenmoku: eight percent iron and a surface you can feel Stoneware
- Shino: a glaze that is mostly feldspar and mostly technique Stoneware
- Wood ash glaze: working with a material that changes every batch Stoneware