Nurtured Clay

Workshop notes, cone 03 to cone 10

Cooling in reduction: how 90 minutes of controlled cooling changes a glaze

Cone 10 Body Stoneware Level Advanced Time 5 hours Filed 1 November 2026

Process parameters · Technique

Clay body
Stoneware
Cone
Cone 10
Temperature
≈ 1305 °C
Difficulty
Advanced
Working time
5 hours
Published
1 November 2026

Tools

  • Pyrometer with a logging output, or a notebook and a timer
  • Damper with a marked position scale
  • Witness cones for cones 9 through 11 to confirm peak temperature
  • A kiln that holds heat — fibre lid and good door seals
  • Heat-resistant gloves and a face shield
  • A shelf of test tiles fired alongside production work to compare cooling effects

Most home kilns cool the same way: shut everything and wait. That natural cooling is fast at the start and slow at the end, and the first 90 minutes below peak temperature are when most of the visual character of a reduction glaze is decided. Controlling that window — holding reduction while the kiln drops from cone 10 to about 1000 degrees — is the difference between a flat tenmoku and one with visible crystal growth.

Cross-section of a 16 cm form: rim 14 cm, belly 16 cm, foot 9 cm.
Vessel cross-section — Section drawn to the rim, belly, foot and height recorded for this entry.
H 16 · Ø14 / Ø16 / Ø9 cm

Why cooling matters more than most people think

A glaze at peak temperature is a liquid. As it cools, crystals nucleate and grow, and the size and number of those crystals determine whether the surface is glossy, satin, or fully crystalline. Slow cooling between cone 10 and 1000 degrees grows crystals; fast cooling freezes the glaze in its liquid structure and gives a glossy surface.

This is why two potters with identical recipes and identical schedules get different results: one cools in eight hours and the other in fourteen. The recipe did not change; the cooling did.

The controlled cool in practice

After the soak at cone 10, close the damper to 10 percent and cut primary air to keep a light reduction atmosphere, then let the kiln fall at 60 to 90 degrees per hour from 1305 to about 1100 degrees. You are not adding heat; you are slowing the loss of it, which means keeping the kiln closed and the damper nearly shut.

Below 1100 degrees, open the damper fully and let the kiln drop naturally to 900. That final stage can be fast — the glaze is already rigid and the crystals have formed. Trying to slow it further mostly wastes time and risks reducing the body again at a temperature where nothing good happens.

Matching the cool to the glaze

Not every glaze wants a slow cool. Iron saturates, oil spot, ash glazes and crystalline mattes all benefit. Clear glazes, most celadons and copper reds do not: a slow cool makes celadon cloudy and a copper red can re-oxidise to green as it drops through 900 degrees with any air available.

A practical arrangement is to fire mixed loads and cool at a moderate 80 degrees per hour to 1100, then open the damper and let it fall. That is slow enough for the iron glazes on the upper shelf and not so slow that the copper reds lose their colour.

Recording what you did

Log the cooling rate alongside the firing schedule, because a cooling change is invisible in the final result until you have two pots to compare. Note the time the kiln passed 1305, the time it passed 1100, and whether the damper was open or closed. After three firings you will have enough data to know which of your glazes responds to cooling and which does not.

A cheap pyrometer with a USB logger costs less than a bag of glaze materials and turns the cooling stage from folklore into a number.

Steps

  1. Soak at cone 10 for 20 minutes with the damper at 50 percent.
  2. After the soak, close the damper to 10 percent and cut primary air to hold a light reduction atmosphere.
  3. Let the kiln fall at 60 to 90 degrees per hour from 1305 down to 1100 degrees.
  4. Record the time and pyrometer reading every 15 minutes through the controlled cool.
  5. Open the damper fully at 1100 degrees and let the kiln fall naturally to 900.
  6. Keep a light reduction below 900 only if firing an oil spot or a crystalline glaze.
  7. Do not open the kiln above 200 degrees Celsius.
  8. Log the cooling rate next to the firing schedule so the two can be compared across firings.

Where it goes wrong

  • Slowing the cool by opening the lid slightly. That adds cold air, which oxidises the surface and chills the ware unevenly.
  • Applying a slow cool to copper reds. They re-oxidise to green as they pass through 900 degrees in air.
  • Cooling too slowly below 900 degrees. Nothing useful happens and the kiln is tied up for an extra six hours.
  • Not recording the rate. Without a number, a result is unrepeatable and you cannot tell a cooling effect from a glaze change.
Symptom and cause
Symptom Cause
Celadon came out cloudy the cool was too slow, allowing micro-crystals to grow in the glaze.
Copper red lost its colour and went green the damper was opened too early, admitting air above 900 degrees.
Oil spot glaze has no spots cooling from cone 10 was faster than 100 degrees per hour.
Glaze result unrepeatable between two firings of the same recipe the cooling rate was not measured or recorded.

Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.

Same cone — Cone 10

← All Techniques