Wax and latex are both resists, and they are not interchangeable. Wax is for the potter who wants a clean, hard-edged line and is willing to apply it at leather-hard; latex is for the potter who needs to peel a resist off a bisqued surface without leaving a residue. Using the wrong one for the job produces either a smeared line or a glaze that refuses to adhere where the latex was.
H 12 · Ø11 / Ø11.5 / Ø6 cm
Wax: applied at leather-hard, for a crisp edge
Wax resist works because the wax sinks into the clay surface and the glaze cannot adhere to it. Apply it at leather-hard, not bone-dry: on bone-dry ware the wax sits on the surface and flakes off during glazing, taking a rim of glaze with it. One coat of hot wax applied with a brush at leather-hard gives a hard, clean line.
Wax the foot ring and the lower 5 mm of every pot before dipping. It saves scraping the foot afterwards, which is where most glaze-related injuries in a studio happen. Melt the wax in a dedicated electric pot; never melt wax over an open flame, and never use the same pot for wax and for food.
Wax on bisque: the second application
Wax also works on bisque, where it is used for decorative resist patterns — dots, stripes and spatter that appear as bare clay against a glaze field. Apply it thicker on bisque than on greenware, because the porous surface drinks the first layer. Two coats with 20 minutes between them gives a pattern that survives a dip.
The line quality on bisque is softer than on greenware, because the wax bleeds slightly along the porous surface. If you want sharp edges on bisque, thicken the wax with 5 percent paraffin and apply it cold with a rubber-tipped tool.
Latex: peel it, do not fire it
Latex resist is liquid rubber. It is applied to bisque, allowed to dry to a rubbery skin in about 15 minutes, and peeled off after glazing. It produces a perfectly clean edge with no residue, and it can be applied over an already-glazed surface to mask a pattern before a second glaze dip.
Two rules. First, never fire latex: it must be peeled before the kiln, and if a piece of it is left in a crevice the burn-out will leave a black scar. Second, do not apply latex to greenware; the water in it will soften the clay surface and the resist will pull clay away when you peel it.
Combining them on one pot
The sequence that works on a single piece: wax the foot at leather-hard and bisque the pot. Apply latex over the areas that get no second glaze, glaze the whole pot, then peel the latex. Then wax over the whole glazed surface, wipe the wax off the areas that get the second glaze, and dip again.
Wax over glaze needs care: the wax must be wiped off, not dissolved, or it will leave a greasy film that repels the second glaze at exactly the edges you wanted sharp. Use a rag dampened with water, wipe once in one direction, and do not go back over the area.
Steps
- Wax the foot ring and the lower 5 mm of the pot at leather-hard, using hot wax and a flat brush.
- Bisque the pot as normal, then apply latex resist to any area that should stay free of the second glaze.
- Let the latex dry to a rubbery skin, about 15 minutes, and apply the first glaze to the whole pot.
- Peel the latex off in one slow movement, pulling back over itself rather than away from the surface.
- Wax over the entire glazed surface with hot wax if a second glaze is planned.
- Wipe the wax off the second-glaze area with a damp rag in a single direction, without going back over it.
- Dip the second glaze and peel or wipe any remaining resist before the kiln.
- Never fire latex — check the foot ring and any crevices for residue before loading.
Where it goes wrong
- Waxing bone-dry ware. The wax flakes during dipping and the flakes carry glaze onto the foot.
- Firing a piece with latex still on it. The burn-out leaves a black scar that cannot be removed.
- Applying latex to greenware. It pulls clay off when peeled and leaves a cratered surface.
- Wiping wax back over an area you have already wiped. The second pass smears the film rather than removing it.
| Symptom | Cause |
|---|---|
| Glaze flaking off in a ring above the foot | wax was applied to bone-dry ware and lifted during the dip. |
| Black scar on the fired surface | latex residue left in a crevice and burned out in the kiln. |
| Ragged edge on a resist pattern | the wax was too thin, or the pot was too wet when it was applied. |
| Second glaze crawled at the edge of a masked area | the wax was smeared rather than wiped, leaving an oily film. |
Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.
Same cone — Cone 6
- Centering a 1 kg ball: wheel speeds, hand positions and the wobble test Stoneware
- Glaze thickness by the numbers: specific gravity, dip seconds and grams per area Stoneware
- Reading a glaze fault: six defects and what actually causes them Stoneware
- Loading a kiln so the top shelf and the bottom shelf match Stoneware