Nurtured Clay

Workshop notes, cone 03 to cone 10

Loading a kiln so the top shelf and the bottom shelf match

Cone 6 Body Stoneware Level Intermediate Time 1 hour 15 minutes Filed 27 October 2026

Process parameters · Technique

Clay body
Stoneware
Cone
Cone 6
Temperature
≈ 1222 °C
Difficulty
Intermediate
Working time
1 hour 15 minutes
Published
27 October 2026

Tools

  • Witness cones in the range being fired
  • Kiln shelves, three props per shelf
  • Spirit level for checking shelves
  • Damp sponge for wiping feet
  • Kiln wash applied and rubbed smooth
  • Stilts for the few pieces that need them
  • A notebook with a sketch of each firing layout

A kiln is not an oven. The bottom shelf of a typical electric kiln runs two cones cooler than the top, and if you load without accounting for that, half the pots come out under-fired and half come out over-fired. Loading is the single highest-leverage variable a potter controls, and it costs an hour of planning rather than a new glaze recipe.

Cross-section of a 12 cm form: rim 13 cm, belly 14 cm, foot 7.5 cm.
Vessel cross-section — Section drawn to the rim, belly, foot and height recorded for this entry.
H 12 · Ø13 / Ø14 / Ø7.5 cm

Knowing your kiln's gradient

Before loading anything important, fire an empty kiln with witness cones on the bottom, middle and top shelves. Most 45 litre electric kilns show about two cones of difference top to bottom; larger kilns show more. Write the numbers on the kiln wall with a marker: it is the most useful piece of information about the kiln you will ever have.

Then place work deliberately. The shelf that runs hot is where the glazes that need heat go — iron saturates, tenmoku, anything that benefits from extra maturity. The cool shelf is for copper reds and pale celadons, which go muddy or colourless when over-fired.

Spacing and thermal mass

Leave 1 to 2 cm between pieces and 2 cm between the work and the kiln wall. Closer than that and the ware either touches during firing as the glazes expand, or shades the thermocouple and gives a false reading.

Load the same shelf with pieces of similar wall thickness. A shelf holding 4 mm cups next to a 25 mm sculpture will fire unevenly, because the heavy piece absorbs heat and delays the shelf's rise. Put the thick work on the shelf that runs hottest and add a soak to the schedule.

Supporting glazed work

Wipe the foot of every glazed piece down to bare clay with a damp sponge, 3 to 5 mm up the wall. Any glaze on the foot ring becomes a weld to the shelf, and freeing a welded pot destroys both it and the shelf.

Stilt the pieces that need it — small marks are easier to grind off than a welded foot is to break free — but use stilts sparingly. Each stilt point is a small thermal mass that can pull a mark into the glaze. Shelves with kiln wash applied fresh and rubbed smooth are better than stilts for anything over 10 cm.

The furniture layout

Put the largest and heaviest pieces on the bottom shelf for stability, and the smallest on the top. Use three props per shelf, not four: three points define a plane and four will rock if the shelf is slightly warped. Check each shelf with a spirit level after the props are in place — a shelf that rocks will tip a piece over during the firing.

Do not use the top of the kiln as extra shelf space unless the lid has a separate short section. The lid area runs hot and unevenly, and it is where the elements are closest to the ware.

Steps

  1. Fire an empty kiln once with witness cones on bottom, middle and top shelves and record the gradient on the kiln wall.
  2. Group work by glaze type and assign each group to a shelf according to whether it needs more or less heat.
  3. Wipe the foot of every glazed piece down to bare clay with a damp sponge.
  4. Place large heavy pieces on the bottom shelf and small light pieces on top.
  5. Use three props per shelf and check the shelf with a spirit level before loading onto it.
  6. Leave 1 to 2 cm between pieces and 2 cm between the work and the kiln wall.
  7. Load each shelf with pieces of similar wall thickness and note any thick pieces so a soak can be added.
  8. Record the layout in a notebook against the firing number so the results can be traced back.

Where it goes wrong

  • Loading without knowing the gradient. It makes any glaze test meaningless, because the result depends on where the tile sat.
  • Using four props per shelf. Four points always rock; three define a plane.
  • Wiping the foot hurriedly while the pot is still damp. The glaze smears down and re-covers the area you just cleaned.
  • Crowding the top shelf because everything has to fit. A crowded top shelf fires hot and slow, which changes the glaze result.
Symptom and cause
Symptom Cause
Half the pots under-fired and half over-fired in the same firing the kiln gradient was not accounted for in the loading plan.
Pot welded to the shelf glaze was left on the foot ring during wiping.
Shelf tipped during the firing four props instead of three, or the shelf was not levelled before loading.
Glaze colour differs between two identical pots they were on shelves with different thermal mass, one next to heavy work and one not.

Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.

Same cone — Cone 6

← All Techniques