Copper gives red in reduction and green in oxidation, and it is the colour that most often surprises potters because a kiln that is only slightly reduced can turn a green glaze into a muddy brown-green without anyone touching the recipe. At cone 04, 3.5 percent copper carbonate in a lead-free frit base gives a clean turquoise, provided the firing is genuinely oxidising from start to finish.
H 11 · Ø13 / Ø14 / Ø7 cm
Base
A low-fire transparent base with copper carbonate added for a clear turquoise green in oxidation. The same base with 0.3 percent cobalt gives the blue of the other low-fire recipe in this library.
| Material | Parts | Share |
|---|---|---|
| Frit 3124 | 40 | 41.5% |
| Silica (SiO₂) | 20 | 20.7% |
| Whiting (CaCO₃) | 15 | 15.5% |
| EPK Kaolin | 15 | 15.5% |
| Copper Carbonate (CuCO₃) | 3.5 | 3.6% |
| Bentonite | 3 | 3.1% |
| Total charge | 96.5 |
Fired surface
A bright, slightly opaque turquoise with darker green where it pools and a paler, almost yellow-green edge where it thins over a rim. Copper at low fire in oxidation is a reliable green as long as the kiln is genuinely oxidising.
Amount, and what it does at each level
Copper carbonate is about 55 percent copper by weight. At 1 percent in this base the glaze is a pale blue-green; at 3.5 percent it is a solid turquoise; at 6 percent it goes dark green with a metallic sheen at the edges, which is unstable and sometimes rubs off. The working range for a food-safe surface is 2 to 4 percent.
Above 5 percent, copper can be released from the glaze into acidic food. This is worth taking seriously: use this glaze on the outside of vessels, or on decorative pieces, and use the cobalt version or a clear on any surface that will hold food.
Why oxidation matters so much
In a reducing atmosphere, copper oxide converts to copper metal or copper(I) oxide, which is red or black. That change can happen in the top 2 mm of a glaze in a matter of minutes. A kiln sharing a flue with another kiln, a kiln with a blocked vent, or a kiln loaded so densely that the air cannot circulate will all produce a green glaze that comes out brown.
The practical precautions: fire this glaze in a well-ventilated kiln, keep the bottom vent open until 600 degrees, leave 2 cm between pieces, and never fire it in the same load as a reduction firing. If you have a gas kiln, this is an electric-kiln glaze.
Copper and the kiln shelf
Copper glazes are volatile and can deposit a pink or green film on any nearby unglazed surface, including shelf boards and the underside of pieces stacked above. This is harmless but unsightly, and on a bare shelf it builds up over time. Fire copper glazes on a washed shelf and keep that shelf for copper.
The same volatility means you should not fire copper green in the same load as a white glaze you need to stay white. The white will pick up a green or pink cast on its exposed edges, and there is no way to remove it after firing.
Mixing and applying
Copper carbonate disperses easily compared to chrome, so it can be added dry to the water with the other materials. Sieve to 80 mesh and dip for one second to reach a 0.4 mm deposit. Thicker than 0.6 mm the green goes dark and the surface loses its brightness.
This glaze crazes on some earthenware bodies because the frit base has a high expansion coefficient. Test it on tiles first, and if it crazes, add 3 percent silica to reduce the expansion. If you are using this on a functional piece, one crazing test tile is worth more than any amount of speculation.
Steps
- Weigh the five base materials with the bentonite and combine them dry.
- Add the copper carbonate to the mixing water and stir until dispersed, then add the dry materials.
- Mix for five minutes with a drill and paddle, then adjust to 1.40 specific gravity.
- Sieve through 80 mesh and add 0.2 percent Epsom salts if it settles quickly.
- Dip test tiles for one second and fire to cone 04 in a well-ventilated oxidation firing.
- Check the fired tile under a loupe for crazing before committing a production load.
- Add 3 percent silica if the tile crazes, and re-test on a new tile.
- Fire copper pieces on a dedicated washed shelf, keeping 2 cm between them and any white glazed work.
Where it goes wrong
- Firing in a slightly reduced kiln. The green goes brown and the recipe gets blamed.
- Going above 5 percent copper on a food surface. Copper can be released into acidic food.
- Firing copper in the same load as a white you need to stay white. The volatility will tint it.
- Skipping the crazing test on a new body. The frit base is high-expansion and will craze on some clays.
| Symptom | Cause |
|---|---|
| Green turned brown or grey-green | the firing was reduced somewhere between 600 and 900 degrees. |
| White glaze in the same load has a pink cast | copper volatility; fire copper loads separately. |
| Fine crazing across the whole surface | the frit base is a poor fit on this body; add 3 percent silica and re-test. |
| Dark green with a metallic sheen that rubs off | copper level above 5 percent; reduce to 3.5. |
Recipe and schedule numbers here were recorded on the workshop’s own kiln. A different kiln, a different thermocouple position or a different clay batch will move the result, so treat every firing schedule as a starting point and keep your own log beside it.